← Back to Patent Explorer
US4496507A Expired / Lapsed US ⏱️ 0.0 years remaining

Production of string-like polytetrafluoroethylene

Assignee: Sumitomo Electric Industries Ltd
•
Filing: 1982-07-02
•
Granted: 1985-01-29
•
Expires: 2002-07-02
📄 Original PDF 🌐 Google Patents 🔄 Sync Now

Abstract

Abstract A process for producing a tube or rod of a polytetrafluoroethylene is described. The process comprises molding a polytetrafluoroethylene containing a liquid lubricant into a tube or rod by a paste process, removing the liquid lubricant, stretching the tube or rod in the lengthwise direction, and thereafter, by sintering the stretched tube or rod at a temperature of at least 327 DEG C. wherein the stretching of the tube or rod is carried out by the use of at least one pair of heating rolls which are each provided with a plurality of grooves. The process provided uniform stretching making it possible to produce a tube or rod with very small internal diameter.

Inventors

  • 👤 Koichi Okita
  • 👤 Shigeru Asako

Bibliographic Details

Application Number —
Jurisdiction US
Data Source google_patents
Last Synchronized 2026-10-23 09:10
CPC Classifications
D; D01; D01F; D01F6/00; D01F6/02; D01F6/08; D01F6/12; B; B29; B29C; B29C67/00; B29C67/20; B29C67/205; D01D; D01D5/00; D01D5/12; D01D5/16; D01D5/24

Claims Analysis

Total Claims: 4
Claim 1
Independent Claim 223 words
A process for producing a string-like porous material of a polytetrafluoroethylene, comprising the steps of: molding polytetrafluoroethylene into a string-like shape, the polytetrafluoroethylene containing a liquid lubricant, the molding being performed by a paste process: removing the liquid lubricant; providing a low speed set of heating rolls and a high speed set of heating rolls, wherein the heating rolls are each provided with a plurality of grooves, and the temperature of the low speed heating rolls is higher than the temperature of the high speed heating rolls; placing the molded polytetrafluoroethylene on the low speed pair of heating rolls by threading it in a FIG. 8 configuration around the low speed rolls and within the grooves thereof; placing the molded polytetrafluoroethylene on the high speed pair of heating rolls by threading it in a FIG. 8 configuration around the high speed rolls and within the grooves thereof; rotating each of the high speed pair of rolls at the same speed and each of the low speed pair of rolls at the same speed, the high speed pair of rolls being rotated faster than the low speed pair of rolls to create a uniform compression force during the stretching, the force being applied in the peripheral direction of the string-like material; sintering the stretched string-like material at a temperature of 327° C. or more.
Claim 2
Dependent Claim 223 words
A process for producing a string-like porous material of a polytetrafluoroethylene, comprising the steps of: molding polytetrafluoroethylene into a string-like shape, the polytetrafluoroethylene containing a liquid lubricant, the molding being performed by a paste process: removing the liquid lubricant; providing a low speed set of heating rolls and a high speed set of heating rolls, wherein the heating rolls are each provided with a plurality of grooves, and the temperature of the low speed heating rolls is higher than the temperature of the high speed heating rolls; placing the molded polytetrafluoroethylene on the low speed pair of heating rolls by threading it in a FIG. 8 configuration around the low speed rolls and within the grooves thereof; placing the molded polytetrafluoroethylene on the high speed pair of heating rolls by threading it in a FIG. 8 configuration around the high speed rolls and within the grooves thereof; rotating each of the high speed pair of rolls at the same speed and each of the low speed pair of rolls at the same speed, the high speed pair of rolls being rotated faster than the low speed pair of rolls to create a uniform compression force during the stretching, the force being applied in the peripheral direction of the string-like material; sintering the stretched string-like material at a temperature of 327° C. or more.
Claim 3
Dependent Claim 40 words
A process for producing a string-like porous material of a polytetrafluoroethylene, as claimed in claim 1, wherein the low speed heating rolls are maintained at a temperature at least 50° C. higher than the high speed pair of heating rolls.
Claim 4
Dependent Claim 73 words
A process for producing a string-like porous material of a polytetrafluoroethylene, as claimed in claim 1, wherein the temperature of the low speed pair of heating rolls are maintained at a temperature of from 250° C. up to the melting point of the polytetrafluoroethylene, and the temperature of the high speed pair of heating rolls are maintained at a temperature at least 70° C. lower than the temperature of the low speed roll.

References Cited (Backward Citations)

DE1410366A1 Cited
US3953566A Cited
US4248924A Cited

USPTO Annuity & Maintenance Windows

Annuity Stage Window Opens Payment Deadline Surcharge Period Until Estimated Fee Status
3.5 Years (Year 4) 1988-01-29 1988-07-30 1989-01-29 $2000.00 Window Closed / Lapsed
7.5 Years (Year 8) 1992-01-29 1992-07-30 1993-01-29 $3760.00 Window Closed / Lapsed
11.5 Years (Year 12) 1996-01-29 1996-07-30 1997-01-29 $7700.00 Window Closed / Lapsed

Assigned Categories & Tags

No categories assigned to this patent yet.

Assign Category Tag